>Hoping to see results from other participants too,
>before the publication of the official comparison.
>
>Best,
>
>Armel Le Bail

Good Idea!

      Size-Strain Round Robin results for CO2 sample

Method: Rietveld-refinement using Modified Thompson-Cox-Hastings
profile function with the Gaussian and Lorentzian FWHM defined as:

FWHMG = (Utan2q + Vtanq + Z/cosq2 + W)1/2

FWHML = X tanq + Y/cosq

Computer Program: Local modification of DBWS

   Results of fitting data from the University of Le Mans 

"Instrumental standard": 
X = 0.0379(8), Y = 0.0116(7), W = 0.00152(5), U=V=Z=0

R-factors: Rwp = 0.110, Rp = 0.074, RB = 0.012

"Broadened sample":
X = 0.080(2), Y = 0.149(2), Z = 0.0396(7), W = 0.00152, U=V=0

R-factors: Rwp = 0.069, Rp = 0.050, RB = 0.036

Calculated volume-weighted size Dv = 273 �


  Results of fitting data from the ESRF BM16 beamline, Grenoble

"Instrumental standard": 
Y = 0.00346(3), W = 0.000021(1), U=V=Z=X=0

R-factors: Rwp = 0.145, Rp = 0.090, RB = 0.015

"Broadened sample":

X = 0.019(2), Y = 0.0477(3), Z = 0.00214(4), W = 0.000021, U=V=0

R-factors: Rwp = 0.040, Rp = 0.029, RB = 0.018

Calculated volume-weighted size Dv = 259 �


Contact address:

Leonid A. Solovyov
Institute of Chemistry and Chemical Technology
K.Marx str. 42
660049, Krasnoyarsk
RUSSIA
E-mail: [EMAIL PROTECTED]