-----Original Message----- From: Anthony Manerbino <[EMAIL PROTECTED]> To: '[EMAIL PROTECTED]' <[EMAIL PROTECTED]> Date: ���������, ������� 23, 2000 08:18 Subject: TiB2 crystal structure >Dear Rietveld list subscribers, > > Does anyone know where I could find a publication with any information on >the structure of TiB2? > >Cheers, >Anthony Manerbino See Z.Anorg.Allg.Chem., 620(1994)1175 Space Group: P6/mmm; a=3.031, c= 3.238 Ti (1a) 0 0 0 B (2d) 1/3 2/3 1/2 Good luck! K.Petrov
- TiB2 crystal structure Anthony Manerbino
- RE: TiB2 crystal structure Peter Y. Zavalij
- Virus? Kovacheva
- Virus? Luis Rodriguez