> Dear Stephen, > I have prepared XPD-standard Y2O3 by firing Y2O3 (99.999) from Aldrich > at 1200 �C for 72 hs. (as done in 41-1105 PDF card). > I would also like to ask the other list members if anyone has calibrated > the size-strain broadening of Y2O3 against LaB6, because I have no > access to LaB6 and I've heard that yttria gives broader lines. > Thanks > Leopoldo
>From Y2O3 annealed at around 1200 degC, and using fundamental parameters peak fitting in XFIT (BGMN and Topas are currently maintained programs), I get around 3300 Angstrom for crystallite size - and near zero strain (using the size/strain modelling defaults in XFIT). Though don't have a comparison with LaB6. What is the certificate crystallite size and strain value for NIST LaB6 - via Google, the NIST website seems to be giving a problem finding this out? http://ois.nist.gov/srmcatalog/certificates/view_cert2pdf.cfm?certificate=660a Error Occurred While Processing Request Error Diagnostic Information An error has occurred. HTTP/1.0 404 Object Not Found Lachlan -- ----------------------- Lachlan M. D. Cranswick Contact outside working hours / Coordonnees en dehors des heures de travail: E-mail / courriel: [EMAIL PROTECTED] Home Tel: (613) 584-4226 Mobile/Cell: 613 401 3433 WWW: http://lachlan.bluehaze.com.au/ P.O. Box 2057, Deep River, Ontario, Canada, K0J 1P0 (please use clear titles in any Email - otherwise messages might accidentally get put in the SPAM list due to large amount of junk Email being received. If you don't get an expected reply to any messages, please try again.) (Essayez d'utiliser des titres explicites - sans quoi vos messages pourraient aboutir dans un dossier de rebuts, du fait de la quantite tres importante de pourriels recue. Si vous n'obtenez pas la reponse attendue, merci de bien vouloir renvoyer un message.)