Dear Frantisek,
your question refers to the application of spherical harmonic models for PO description/correction in Rietveld QPA of minerals in multiphases samples. My five cents:

The spherical harmonic models do not have any direct physical meaning. They just fulfill the symmetry of the Laue class, and they can only be applied if the geometry of you diffraction experiment is rotational symmetric (e.g. in Bragg-Brentano geometry with flat (rotating) sample and point detector). The models can work successfully in QPA only if the normalization of the scale factors works correctly. Improved Rwp is not a criterion for good/bad model decision.

From practical point of view, the models can be applied only if there is enough information in the powder pattern (measured peak intensities in different hkl directions), in relation of the degrees of freedom (number of refineable parameters what are introduced by the the models).

The effective number of parameters of the several orders of these functions and related to the Laue classes is discussed, for example, in S. Matthies and K. Helming. General Consideration of the loss of information on . . . . phys. stat. sol. (b), 113:569–582, 1982, or table 1 in J. Bergmann, T. Monecke, and R. Kleeberg. Alternative algorithm for the correction of preferred orientation in rietveld analysis. J. Appl. Cryst., 34:16–19, 2001., cited from Bunge, H. J. (1993). Texture Analysis in Material Science: Mathematical Methods. GoÈ ttingen: Cuvillier. Accordingly, you need higher orders of SH's for higher symmetric materials. My personal rule of thumb for minerals is order 2 for triclinic and monoclinic, 4 for orthorhombic/hexagonal/tetragonal, and 6 for cubic phases. Doing so, you introduce maximum of 6 effective correction parameters but still have a correction effect. (For comparison, for triclinic structure a 6. order would introduce 28 (!) effective parameters, "with enough parameters you can fit...".)

To reduce the danger of over-parametrization by such models, the BGMN software automatically deactivates SH models when not enough peaks or not enough intensity is in the patterns as found in the first refinement cycles. The fit becomes worse of course, but totally nonsense QPA results are avoided. However, even by this strategy correction models may fail in QPA, when extreme correction factors are calculated maybe by correlation problems etc.. Thus, one should have a look on the hkl specific correction factors (m.r.d.'s). Of course, negative intensities should not appear at all, if the software uses a quadratic or exponential form, like BGMN. But extremely sharp PO may still be a significant problem for SH models. Personally, I don't trust my QPA results when correction factors of < 0.4 or > 3 appear in a QPA refinement. In such cases we try to prepare a better (more randomly oriented) powder sample and repeat the analysis.

Best regards

Reinhard



Am 17/01/2017 um 16:33 schrieb Laufek František:

Here it is:

J. Appl. Cryst. (2005), 38, 158-167.

Powder Diffraction (2009), 24(4), 315-326.

Frantisek

*From:*[email protected] [mailto:[email protected]] *On Behalf Of *Cline, James Dr. (Fed)
*Sent:* Tuesday, January 17, 2017 2:54 PM
*To:* Laufek František
*Cc:* [email protected]
*Subject:* RE: order of Spherical Harmonics for correction of PO

OK, can you list the citations for the papers in question?

Jim

James P. Cline
Materials Measurement Science Division
National Institute of Standards and Technology
100 Bureau Dr. stop 8520 [ B113 / Bldg 217 ]
Gaithersburg, MD 20899-8523    USA
[email protected] <mailto:[email protected]>
(301) 975 5793
FAX (301) 975 5334

*From:*[email protected] <mailto:[email protected]> [mailto:[email protected]] *On Behalf Of *Laufek František
*Sent:* Tuesday, January 17, 2017 8:30 AM
*To:* 'Sitepu, Husinsyah' <[email protected] <mailto:[email protected]>>
*Cc:* [email protected] <mailto:[email protected]>
*Subject:* RE: order of Spherical Harmonics for correction of PO

Dear Husin,

Thank you very much for the papers!

Best Regards,

Frantisek

*From:*Sitepu, Husinsyah [mailto:[email protected]]
*Sent:* Tuesday, January 17, 2017 6:37 AM
*To:* František Laufek
*Subject:* RE: order of Spherical Harmonics for correction of PO

Classification:*Non-Business Use*

*Dear Dr Laufek,*

**

*The enclosed articles are probably useful information to answer your question.*

**

*All the best for the New Year.*

**

*Husin*


//

*/Husin Sitepu, PhD/*

/Saudi Aramco /

/Research and Development Center (R&DC)/

/Technical Service Division (TSD)/

/Advanced Analysis Unit (AAU)/

/Room: GB-110, Bld. 2296/

/P.O. Box 62, Dhahran 31311, Saudi Arabia/

/Phone: (966) <Tel:%28+966%29> 13 876 3050/

/Email: [email protected] <mailto:[email protected]> /

/Links at Google Scholar <http://scholar.google.com/citations?user=cUTV8HkAAAAJ&hl=en>///

/ResearchGate <https://www.researchgate.net/profile/H_Sitepu/stats> /

/
/

This email has been classified as Non-Business Useby *Sitepu, Husinsyah* on Tuesday, January 17, 2017 8:37:00 AM

**

*From:*[email protected] <mailto:[email protected]> [mailto:[email protected]] *On Behalf Of *František Laufek
*Sent:* Monday, January 16, 2017 12:11 AM
*To:* [email protected] <mailto:[email protected]>
*Subject:* order of Spherical Harmonics for correction of PO

/*EXTERNAL: This is an external email received from the Internet. Report this message to [email protected] <mailto:[email protected]> if the email contains any suspicious content.*//**/

/*
------------------------------------------------------------------------
*/

Normal 0 21 false false false CS X-NONE X-NONE

Dear colleagues,

I use Rietveld method for quantitative phase analysis. I use Topas 5 and now I have started using

Spherical Harmonics for correction of preferred orientation (instead of March-Dollas correction).

I mainly collect data in Bragg-Brentano geometry; samples are usually prepared by front or side-loading.

My question is: Which order of Spherical Harmonics do you recommend to use for the purpose of QPA? i.e. for mineral phases like calcite, mica, feldspars, plagioclase, kaolinite?

(Most atomic position are usually fixed, refined are only scale factors, unit-cell parameters, size, Debye-Waller parameters…).

I know that using high order Spherical Harmonic may lead to nice fits, however with meaningless results and therefore the high orders should be used with cautions.

I observe the drop of Rwp when introducing the Spherical Harmonics correction and when it becomes insignificant, than I reduce the order. E.g. for calcite, it is order of 2, for kaolinite order of 4 (i.e. using higher order lead only to insignificant drop of Rwp).

Your suggestions, experiences and comments are welcome.

Frantisek Laufek

Czech Geological Survey,

Prague

Czech Republic

------------------------------------------------------------------------


The contents of this email, including all related responses, files and attachments transmitted with it (collectively referred to as “this Email”), are intended solely for the use of the individual/entity to whom/which they are addressed, and may contain confidential and/or legally privileged information. This Email may not be disclosed or forwarded to anyone else without authorization from the originator of this Email. If you have received this Email in error, please notify the sender immediately and delete all copies from your system. Please note that the views or opinions presented in this Email are those of the author and may not necessarily represent those of Saudi Aramco. The recipient should check this Email and any attachments for the presence of any viruses. Saudi Aramco accepts no liability for any damage caused by any virus/error transmitted by this Email.



++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <[email protected]>
Send commands to <[email protected]> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++



--
TU Bergakademie Freiberg
Dr. R. Kleeberg
Mineralogisches Labor
Brennhausgasse 14
D-09596 Freiberg

Tel.    ++49 (0) 3731-39-3244
Fax. ++49 (0) 3731-39-3129

++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <[email protected]>
Send commands to <[email protected]> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to