Hi,

Assuming average CoKa wavelength of 1.7902 angstrom, using the values in the 
Table 1 of E975-22, below R values can be used:


Alpha Fe:   R
110     149.64
200     19.555
211     40.257
220     18.233


Gamma Fe:  R
111     111.275
200     48.980
220     25.906
311     12.187





--

Dr. Xiaodong (Tony) Wang
Senior Research Infrastructure Specialist (XRD)
Central Analytical Research Facility (CARF)   |  Queensland University of 
Technology
Address: Level 6, P Block, Gardens Point campus, 2 George St Brisbane QLD 4000
Tel: +61 7 3138 1904  |   Mob: 0452 571 680
Email:   [email protected]   |   Web: www.qut.edu.au/ife/carf



At 2026-03-10 02:32:55, "Nelson Duarte" <[email protected]> wrote:

Dear colleagues,

I am trying to calculate the retained austenite content according to ASTM E975 
using cobalt radiation.

Does anyone have calculated the theoretical intensity values of the main 
ferrite and austenite peaks using  cobalt radiation?

Thank you in advance.

Best regards,

Nelson

 
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <[email protected]>
Send commands to <[email protected]> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to