Thanks to those that replied at least this is a start on a little known subject. YES i know this is silver list, But it is a colloid ? The knowledge base is growing.. I tried making copper like c/s was not pleased with the result, must be another way.
1: Firstly if making precision anything, remove as many variables as possible Water. 1: Rain (direct) into glass, not off the roofing, or as in my case pure spring water gives the best results. If you start with bad water you will always have bad water, Proved this by first making a still.,(Beginner of course) using a tin plated boiler into a stainless condenser, got a tinny taste, tried aluminium, got cloudy results making c/s. Under those conditions, spring water tasted best, I now use all stainless, But pyrex glass would be better I think. Commercial distiller machine water, tastes of plastic, some that i sampled anyway. didnt use it. Once asked some sellers of these machines, (Trick Question) If I were to put Cyanide (Possum poison) in the water and you were to distill it in your marvellous machine, will you drink the distilled water ? Answers were allways NO! Storage of distilled water: Use washed glass only (rinse well ) , New plastic bottles are contaminated, oil mist particles if blow moulded, also some very toxic mould release chemicals can be present. (silicone ?) used bottles are probably not as bad. Although I have read somewhere that contamination from the plastic itself is possible. Temp: This has a definite effect on quality and speed, and current flow after much experimentation I have found a constant temp of 110>F works best, dont preheat in microwave, stand your bottles on a warmer pad and adjust water temp. takes a little time to set up. You could use a stove element but this is dangerous and difficult to repeat reliably and if the glass should break or you accidently spill it. you got problems c/s possibly wont fix. Warm your next batch of water at the same time. Temp influences current flow markedly. Constant current: I am making c/s at only 7 volts using pulsed dc. using about 2oz starter c/s in to 28oz. Glass Jar. Will make 28oz in about 2-3 hours, (sorry never bothered to time it exactly) no sediment or floating particles. no filtering. my power supply can put out 6 amps, current actually used is very dependant on the area of electrode immersed in the water. What this means is the process will only draw as much as it needs until it reaches runaway. (low resistance) With the use of a line current meter and monitor. (Few diodes and a transistor,and relay.) My unit switches off automatically when this current flow reaches 8ma, (adjustable) this means a set and forget, no overcurrent possible, same result every time. More than 10ma should never be required. At 8ma current flow my ppm is correct, and the process is complete. You would have to work out your own completion ppm and current flows as this will depend on your electrode length, size and spacing. small diameter wire, under 1mm is not suitable. At least 1.2mm+ is needed. otherwise your surface area to space available in a 28oz jar just wont work out very well. Bar shaped electrode would be better, but run whatcha brung. Happy Fiddling. PY -- The silver-list is a moderated forum for discussion of colloidal silver. To join or quit silver-list or silver-digest send an e-mail message to: [email protected] -or- [email protected] with the word subscribe or unsubscribe in the SUBJECT line. To post, address your message to: [email protected] List maintainer: Mike Devour <[email protected]>

