What temperature are you developing at?  Have you tried moving down to 65F
or so?

Are you using a tank or roller transport?

If you're using a polyester base, try an acetate base instead, which has
better adhesion.

Commercial emulsions use an adhesive layer.  You could try making a really
dilute (1/2 percent) solution of 3-amino-propyltriethoxysilane in alcohol
and coating with that.  Eastman Chemicals should have it, or you could ask
Photographer's Formulary.