Thermal exp. coefficient for Pd  within temperature interval 20-1100K found
in a russian handbook "Physical constants" ed. Grigoriev and Mejlihov,
Moskva 1991.

temperature[K]  20     30      50     100     200      300      400     500
600    800   1100

alpha 10-6/K     0.5   1.12   3.57   7.95   10.84   11.75   12.48   13.2
13.9   15.3   17.4

Good luck!