> Some investigators working on metals have found an expansion of cell (that
> is, an increase in the lattice parameters) when grain sizes change from
> micrometers to nanometers. Could anyone provide me a reason for that
> behaviour?.

The atoms at the suface of a solid are coordinated differetly than those
in the bulk, i.e. they feel other atoms of the same solid on one side and
either vacuum, gas or some impurities on the other side. 
Depending on the nature of the interatomic forces the surface atoms are
either pulled towards the crystal bulk or relaxed outwards. Consequently
the interatomic distances at the surface are different from those in the
bulk. In case of nano-sized crystallites the surface atoms constitute a
considerable fraction of the total crystal volume. Since the x-ray
investigations probe the average interatomic distances, the numbers you
get from x-ray data for the lattice parameters change as the crystal size
becomes smaller an smaller. For extended discussion see:
J. Phys.: Condens. Matter 16 (11 February 2004) S353-S377
High pressure x-ray diffraction studies on nanocrystalline materials
B Palosz et all
http://stacks.iop.org/0953-8984/16/S353

Stan

Reply via email to