My samples are cements (fine samples with 30 microns) and don't need micronize 
its. The problem in my refinements is that periclase quantified with fixed slit 
is bigger than MgO by Fluorescence, and its impossible. Ex:

 

Periclase with fixed slit: 7,14%

MgO by XRF = 6,84%

 

We know that part of MgO (1,5-2,0%) go to the structure of C3S an C2S phases, 
so periclase expected in this sample is 4,8% - 5,3%. If we consider this, the 
errors of refinement is not  very slim.

 

Sorry for my bad English!!!

 

regards

 

===========================================

José Carlos Cordeiro

Diretoria Técnica - Laboratório Central

Centro Técnico - Curitiba 

Rodovia PR-092, 1303, Abranches, 82130-570 Curitiba-PR    

Votorantim Cimentos 

[EMAIL PROTECTED] <mailto:[EMAIL PROTECTED]> 

www.votorantimcimentos.com.br 

Fone: + 55 041 3355-1380 

Fax:   + 55 041 3355-1358

===========================================

-----Mensagem original-----
De: Whitfield, Pamela [mailto:[EMAIL PROTECTED] 
Enviada em: quinta-feira, 29 de maio de 2008 17:40
Para: José Carlos Cordeiro; [email protected]
Cc: Mitchell, Lyndon
Assunto: RE: ADS

 

Hi Jose 

 

Errors in the region of 1wt% aren't unheard of in complex mixtures (and the 
liklihood of the second decimal place being meaningful is very slim).  However 
there are other possible explanations and one in particular comes to mind.

Did you micronize your sample?  If yes then feel free to ignore the following!  
If not then it might be worth thinking about.

 

We did a systematic study on the effect of particle statistics on the 
repeatability of quantitative analysis on one of the NIST cements last year 
(presented at the ICCC in Montreal - should really go somewhere more 
accessible).  We compared different divergence slits, micronized and 
unmicronized samples, spun and static, and remounted/repeated the experiments 3 
times each for real statistics as opposed to esds.  

 

Funnily enough the phase that showed the biggest anomaly in one of the unground 
sample was the periclase - obviously a big (by XRD standards) lump fell into 
the sample from the kiln that made up the NIST batch and made it through the 
mill at the plant.  Without grinding it we got 0.1, 0.1 and 2wt% one series of 
3, versus 0.6, 0.6 and 0.6 wt% (this is from memory so don't don't quote me!) 
for the micronized sample.

This was the result that we should have got theoretically but it was nice to 
see it work in practice, and the periclase did such a nice job for us by 
sticking out like a sore thumb even without a Rietveld analysis!  BTW there was 
no statistically significant difference (95% limits) in the results of the C3S 
and C2S phases between ground and unground samples - mostly because the errors 
in the unground samples were so large!  The minor phases were another matter.  
In the micronized samples the choice of divergence slit size made little 
difference, but with the unground samples they made a significant difference.

 

To cut a long story short it all comes down to particle statistics - with an 
ideal powder the choice of fixed versus variable slits (or even different fixed 
slits) should make no difference (assuming that the Rietveld software can 
handle the difference in profiles).  Moral of the story - sample prep, sample 
prep and more sample prep!

 

Pam

        -----Original Message-----
        From: José Carlos Cordeiro [mailto:[EMAIL PROTECTED] 
        Sent: May 29, 2008 3:53 PM
        To: [email protected]
        Subject: ADS

        I have a Programmable Divergence Slit (incident beam) in my 
difratctometer, that can work in automatic mode (irradiated length) or fixed 
mode (0.5 degree or 1.0 degree etc). What is the best collect mode for Rietveld 
Refinament??

         

        I did refinement two difractograms collected in booth configuration 
(fixed 0.5 degree and automatic mode), the results in the fase "Periclase" 
(cement fase) changed, see below:

         

        Periclase with 0.5 degree = 6.08%

        Periclase wich automatic mode = 7.14%

         

        Note.: The refinement of the difractograms collected with automatic 
mode went converted to fixed mode by software.

         

         

         

        What do you think about this?

         

        regards

         

        ===========================================

        José Carlos Cordeiro

        Diretoria Técnica - Laboratório Central

        Centro Técnico - Curitiba 

        Rodovia PR-092, 1303, Abranches, 82130-570 Curitiba-PR    

        Votorantim Cimentos 

        [EMAIL PROTECTED] <mailto:[EMAIL PROTECTED]> 

        www.votorantimcimentos.com.br 

        Fone: + 55 041 3355-1380 

        Fax:   + 55 041 3355-1358

        ===========================================

         

Reply via email to