Hi All,
 
I have been following this discussion with much interest. For what it's worth, 
I think that you also need to consider issues to do with the data collection 
strategies used. Periclase has a small cubic unit cell and hence has very few 
reflections in a typical scan rang used for QPA in a production environment.
 
If we assume Cu Kalpha radiation and a scan range up to 90deg 2theta, periclase 
has only 5 reflections (and only 2 of these have intensity > 10% I/Io). If Co 
Kalpha is used, then the total number of reflections is 4. In a Rietveld based 
analysis, this is too few reflections to ensure stable refinement of many 
parameters related to periclase. Any minor errors in the periclase model have 
the potential to be reflected in the QPA.  
For example - if there is a little solid solution of Fe in periclase (quite 
possible in this environment) then the relative intensities will vary - try 
doing a calculated pattern in your favourite Rietveld program - below are some 
values for F^2
 
h k l        MgO           (Mg0.95Fe0.05)O        % change
 
1 1 1       10.99                   14.86                        35.2
0 0 2     170.20                 181.39                          6.6
0 2 2     202.72                 215.33                          6.2
3 1 1      38.82                    45.46                        17.1
 
While there is an overall increase in calculated F^2 by the inclusion of Fe, 
more important is the change in relative intensities.
 
To assess whether there is any solid solution present try collecting a pattern 
to the limit of the diffractometer (> 140 deg 2Theta if possible) and refine 
the unit cell parameter for periclase. Then simply apply Vegard's Law.  If the 
cell is indistinguishable from the reported periclase cell, then all of these 
ramblings have been in vain!
 
The issues relating to crystallite size already discussed in this thread are 
especially important since there are too few reflections from periclase to 
'average out' the impact of any intensity abberations - at he very least, spin 
the sample to help minimise this.
 
You can see I have too much time on my hands, but this seems like a good way to 
fill in time in the small hours of the morning while waiting for data to 
collect ( we have some beamtime on the powder diffractometer at the Oz 
Synchrotron) 
 
 
Cheers
 
o----------------------oo0oo---------------------------o
     Ian Madsen
     Team Leader - Diffraction Science
     CSIRO Minerals
     Box 312
     Clayton South 3169
     Victoria
     AUSTRALIA
     Phone +61 3 9545 8785 direct
                 +61 3 9545 8500 switch
                 +61 (0) 417 554 935 mobile
     FAX    +61 3 9562 8919
     Email [EMAIL PROTECTED] <mailto:[EMAIL PROTECTED]>  
o----------------------oo0oo---------------------------o
 

        -----Original Message----- 
        From: [EMAIL PROTECTED] [mailto:[EMAIL PROTECTED] 
        Sent: Sat 31/05/2008 3:37 AM 
        To: Whitfield, Pamela; Kurt Leinenweber; [EMAIL PROTECTED]; 
[email protected] 
        Cc: 
        Subject: RE: RES: ADS
        
        


        Hi all, in this long and interesting discussion I think that Prof.
        Leinenweber has indicated where it is one of the problems in
        quantitative phase analysis. Regards,
        
        --
        ********************************
        Jose M. Amigo
        http://www.uv.es/~amigo/
        ********************************
        
        > Interesting thought and probably worth following up, although it
        sounds like a meticulous and possibly time-consuming study for
        someone or other - any volunteers? :-)
        > Following Deane Smith's methodology you should be able to calculate
        the number of diffracting crystallites per phase for particular
        crystallite sizes and fraction (assuming some sampling volume - I
        vaguely remember his being 20mm^3 or something).  I suppose that
        whether you're using a PSD or 2D detectors as opposed to point
        detectors and the geometry would also have to be taken into account.
        >
        > In our cement experiment the % difference between 0.1% and 2%
        periclase is quite large to say the least.  In terms of practical
        versus theory, we did find that up to a point, the 'real' standard
        deviation from repeated experiments with micronized samples can be
        smaller than the esds calculated by the Rietveld program - a happy
        note for repeatability!  On a less happy note that doesn't mean that
        something like severe microabsorption doesn't come along and mess up
        your accuracy.
        >
        > Pam
        >
        > -----Original Message-----
        > From: Kurt Leinenweber [mailto:[EMAIL PROTECTED]
        > Sent: May 30, 2008 11:11 AM
        > To: Whitfield, Pamela; [EMAIL PROTECTED]
        > Cc: [email protected]
        > Subject: RE: RES: ADS
        >
        > Hi all,
        >
        > This is an interesting discussion of quantitative phase analysis. 
        It sounds to me from what Pam is saying that we can calculate an esd
        for each phase if we know its particle size, and that the relative
        error would be larger for phases in smaller abundance.  If this is
        correct, then you could also repeat the physical experiment several
        times and get a variation of similar magnitude to the one that is
        calculated.  Is this what happens?  Pamela refers to the errors as
        being "worse" for minor phases, but they are what they are, and why
        not estimate them?
        >
        >                               - Kurt
        >
        > -----Original Message-----
        > From: Whitfield, Pamela [mailto:[EMAIL PROTECTED]
        > Sent: Friday, May 30, 2008 7:30 AM
        > To: [EMAIL PROTECTED]
        > Cc: [email protected]
        > Subject: RE: RES: ADS
        >
        > Hi Rheinhard
        >
        > The comments weren't aimed at you in particular!  We've been
        banging our heads against a brick wall about this stuff for some
        time, but not many in the cement community seem to be listening.
        >
        > Anyway - there is a fundamental statistics problem with quantifying
        minor phases (of any symmetry) as the stats get worse with fewer
        diffracting crystallites.
        > The numbers that Deane Smith produced in terms of reproducibility
        of the quartz reflection dealt with a single phase system.  It
        doesn't take much to imagine (or at least I do) that things rapidly
        get worse in a multi-phase system where theoretically every phase
        should consist of a nice random powder, reducing the required average
        particle size even further.  It should follow then that the errors
        obtained with minor phases will be worse than major phases where the
        stats are better even without any other effects.  Maybe my logic is
        flawed but I don't think so!  Having said that it has been
        demonstrated that the situation isn't quite as bad practically as it
        is theoretically.
        >
        > Pam
        >
        > -----Original Message-----
        > From: Reinhard Kleeberg [mailto:[EMAIL PROTECTED]
        > Sent: May 30, 2008 10:10 AM
        > To: Whitfield, Pamela
        > Cc: [email protected]
        > Subject: Re: RES: ADS
        >
        >
        > Hi Pam,
        > maybe a misunderstanding: I did not try to discuss the amount of
        > "amorphous" material in cements. I'm aware of the problem, but a
        > careful  Rietveld analysis with an internal standard should be able
        to
        > determine at least the magnitude of the amorphous part. Even if not
        > (e.g. if profile errors or structural uncertainties of the clinker
        > phases do prohibit a reliable quantification of the amorphous), a
        > systematic error of 7 instead of 5 wt% for a highly symmetric phase
        with
        > well resolved peaks like periclase is neither acceptable nor
        > unavoidable. And in my opinion a careful sample prep, measurement
        and
        > Rietveld analysis (maybe with internal standard) should be able to
        > perform better. I only tried to relativise Lubo's general denial of
        the
        > potential of quantitative phase analysis to reach an accuracy of
        about 1
        > wt%. Maybe I'm simply more optimistic than Lubo ;-)
        > Reinhard
        >
        > Whitfield, Pamela schrieb:
        >
        > > Hi Reinhard
        > > 
        > > Saying the words amorphous content and cement in the same breath
        is
        > > heresy in many circles!  Personally I think that it's a case
        of 'see
        > > no evil, hear no evil'!
        > > Anyway, many moons ago we did yet another study on the amorphous
        > > content in clinkers/cements and they can vary alot - we found up
        to
        > > 20wt% in some.  The amount probably depends on the kiln
        conditions,
        > > alkali metal content and quenching rate.
        > > Anyway don't take my word for it, Lerch and Brownmiller did a
        lovely
        > > bit of work (sadly forgotten) in 1937 using quenching in mercury
        (?!)
        > > and calorimetry yielding amorphous contents in clinker between
        > > 10-28%.  The Ruland method has also been used to show significant
        > > amorphous contents in the various components of cement.
        > > 
        > > In my opinion the cement companies are probably more interested in
        > > consistency rather than accuracy to track changes in their
        process. 
        > > Case in point - strictly speaking the XRF samples should be
        micronized
        > > (or fused) as well as the XRD ones - the XRF errors from the
        matrix
        > > effects of a 30micron cement in a pressed pellet are not exactly
        ideal.
        > > 
        > > I would agree that it's worth trying to push the boundaries of
        QPA.
        > > All is not lost for cements though - I saw the results of a test
        that
        > > Mati Raudsepp did with a very messy synthetic mineral mixture
        that
        > > looked completely ridiculous with the number of phases, but the
        result
        > > matched the weighing figures quite nicely.
        > > 
        > > Pam
        > >
        > > ------------------------------------------------------------------
        ----
        > > --
        > > *From:* Reinhard Kleeberg [mailto:[EMAIL PROTECTED]
        > > *Sent:* Fri 30/05/2008 5:36 AM
        > > *To:* [email protected]
        > > *Subject:* Re: RES: ADS
        > >
        > > Hi Lubo,
        > > the difference between 6 and 7 % MgO is bigger than 15 %
        relatively,
        > > thus the error by wrong re-scaling (e.g. if 10 % "amorphous" are
        > > missing) is smaller than the error discussed. And, if the "true"
        > > content of periclase should be about 5 %, than a measured value
        of 7 %
        > > is worth to be discussed to be a real systematic error. This is
        an
        > > over-estimation by 40 %. In the very past (30 years and more ago)
        > > people who applied single line methods carefully have been able
        to
        > > determine "simple" phases like free lime, quartz, anatase in low
        > > concentrations very accurate (of course after optimizing their
        > > technique), and I believe that such methods are still in use in
        > > routine product control. So I feel it is worth to think about why
        a
        > > Rietveld refinement should perform worse. I agree with you that
        the
        > > cement business is full of dubious advertisement for machines and
        > > methods for accurate QPA. But this is not a reason to finish
        thinking
        > > about  how to improve QPA methods. Best
        > > Reinhard
        > >
        > > Lubomir Smrcok schrieb:
        > >
        > > > Hi,
        > > > I really wonder why do you bother about 1% difference when the
        error
        > > > of the method (XRD, quantitative phase analysis) could reach 10%
        > > > (absolute) ...
        > > > People in the discussions appearing here seem to forget about
        two
        > > things:
        > > >
        > > > i) "quantitative" phase analysis done by rietveld method is
        always
        > > > re-scaled to 100%, i.e. the accuracy of % attributed to the
        > > > individual phase directly depend on %'s attributed to the
        another
        > > > phases present in the mixture (i.e. when you forget or ignore
        one
        > > > phase having 10% share, those %'s are redistributed among the
        other
        > > > phases);
        > > >
        > > > ii) this method completely ignores any amorphous parts (i.e.
        those
        > > > not providing Bragg peaks, to be more exact) - ignores, because
        it
        > > > cannot do anything else about it. Obviously, when you compare
        XRF
        > > > and XRD you can find yourself in troubles as XRF dos not bother
        > > > about the state of the compounds.
        > > >
        > > > Finally, my personal advice. If someone tells you you can
        analyze
        > > > clinkers or even cements by XRD accurately, do not trust him.
        He,
        > > > most probably, thinks of selling you a machine you can hardly
        use
        > > > for this purpose :-) Bad luck if you have already bought it ...
        > > >
        > > > Best,
        > > > Lubo
        > > >
        > > >
        > > >
        > > > On Thu, 29 May 2008, [iso-8859-1] José Carlos Cordeiro wrote:
        > > >
        > > >> My samples are cements (fine samples with 30 microns) and
        don't
        > > >> need micronize its. The problem in my refinements is that
        periclase
        > > >> quantified with fixed slit is bigger than MgO by Fluorescence,
        and
        > > >> its impossible. Ex:
        > > >>
        > > >>
        > > >>
        > > >> Periclase with fixed slit: 7,14%
        > > >>
        > > >> MgO by XRF = 6,84%
        > > >>
        > > >>
        > > >>
        > > >> We know that part of MgO (1,5-2,0%) go to the structure of C3S
        an
        > > >> C2S phases, so periclase expected in this sample is 4,8% -
        5,3%. If
        > > >> we consider this, the errors of refinement is not  very slim.
        > > >>
        > > >>
        > > >>
        > > >> Sorry for my bad English!!!
        > > >>
        > > >>
        > > >>
        > > >> regards
        > > >>
        > > >>
        > > >>
        > > >> ===========================================
        > > >>
        > > >> José Carlos Cordeiro
        > > >>
        > > >> Diretoria Técnica - Laboratório Central
        > > >>
        > > >> Centro Técnico - Curitiba
        > > >>
        > > >> Rodovia PR-092, 1303, Abranches, 82130-570 Curitiba-PR
        > > >>
        > > >> Votorantim Cimentos
        > > >>
        > > >> [EMAIL PROTECTED]
        > > >> <mailto:[EMAIL PROTECTED]>
        > > >>
        > > >> www.votorantimcimentos.com.br
        > > >>
        > > >> Fone: + 55 041 3355-1380
        > > >>
        > > >> Fax:   + 55 041 3355-1358
        > > >>
        > > >> ===========================================
        > > >>
        > > >> -----Mensagem original-----
        > > >> De: Whitfield, Pamela [mailto:[EMAIL PROTECTED]
        > > >> Enviada em: quinta-feira, 29 de maio de 2008 17:40
        > > >> Para: José Carlos Cordeiro; [email protected]
        > > >> Cc: Mitchell, Lyndon
        > > >> Assunto: RE: ADS
        > > >>
        > > >>
        > > >>
        > > >> Hi Jose
        > > >>
        > > >>
        > > >>
        > > >> Errors in the region of 1wt% aren't unheard of in complex
        mixtures
        > > >> (and the liklihood of the second decimal place being
        meaningful is
        > > >> very slim).  However there are other possible explanations and
        one
        > > >> in particular comes to mind.
        > > >>
        > > >> Did you micronize your sample?  If yes then feel free to
        ignore the
        > > >> following!  If not then it might be worth thinking about.
        > > >>
        > > >>
        > > >>
        > > >> We did a systematic study on the effect of particle statistics
        on
        > > >> the repeatability of quantitative analysis on one of the NIST
        > > >> cements last year (presented at the ICCC in Montreal - should
        > > >> really go somewhere more accessible).  We compared different
        > > >> divergence slits, micronized and unmicronized samples, spun
        and
        > > >> static, and remounted/repeated the experiments 3 times each
        for
        > > >> real statistics as opposed to esds.
        > > >>
        > > >>
        > > >>
        > > >> Funnily enough the phase that showed the biggest anomaly in
        one of
        > > >> the unground sample was the periclase - obviously a big (by XRD
        > > >> standards) lump fell into the sample from the kiln that made
        up the
        > > >> NIST batch and made it through the mill at the plant.  Without
        > > >> grinding it we got 0.1, 0.1 and 2wt% one series of 3, versus
        0.6,
        > > >> 0.6 and 0.6 wt% (this is from memory so don't don't quote me!)
        for
        > > >> the micronized sample.
        > > >>
        > > >> This was the result that we should have got theoretically but
        it
        > > >> was nice to see it work in practice, and the periclase did
        such a
        > > >> nice job for us by sticking out like a sore thumb even without
        a
        > > >> Rietveld analysis!  BTW there was no statistically significant
        > > >> difference (95%
        > > >> limits) in the results of the C3S and C2S phases between
        ground and
        > > >> unground samples - mostly because the errors in the unground
        samples
        > > >> were so large!  The minor phases were another matter.  In the
        > > >> micronized samples the choice of divergence slit size made
        little
        > > >> difference, but with the unground samples they made a
        significant
        > > >> difference.
        > > >>
        > > >>
        > > >>
        > > >> To cut a long story short it all comes down to particle
        statistics
        > > >> - with an ideal powder the choice of fixed versus variable
        slits
        > > >> (or even different fixed slits) should make no difference
        (assuming
        > > >> that the Rietveld software can handle the difference in
        profiles). 
        > > >> Moral of the story - sample prep, sample prep and more sample
        prep!
        > > >>
        > > >>
        > > >>
        > > >> Pam
        > > >>
        > > >>     -----Original Message-----
        > > >>     From: José Carlos Cordeiro
        [mailto:[EMAIL PROTECTED]
        > > >>     Sent: May 29, 2008 3:53 PM
        > > >>     To: [email protected]
        > > >>     Subject: ADS
        > > >>
        > > >>     I have a Programmable Divergence Slit (incident beam) in
        my
        > > >> difratctometer, that can work in automatic mode (irradiated
        length)
        > > >> or fixed mode (0.5 degree or 1.0 degree etc). What is the best
        > > >> collect mode for Rietveld Refinament??
        > > >>
        > > >>
        > > >>
        > > >>     I did refinement two difractograms collected in booth
        > > >> configuration (fixed 0.5 degree and automatic mode), the
        results in
        > > >> the fase "Periclase" (cement fase) changed, see below:
        > > >>
        > > >>
        > > >>
        > > >>     Periclase with 0.5 degree = 6.08%
        > > >>
        > > >>     Periclase wich automatic mode = 7.14%
        > > >>
        > > >>
        > > >>
        > > >>     Note.: The refinement of the difractograms collected with
        > > >> automatic mode went converted to fixed mode by software.
        > > >>
        > > >>
        > > >>
        > > >>
        > > >>
        > > >>
        > > >>
        > > >>     What do you think about this?
        > > >>
        > > >>
        > > >>
        > > >>     regards
        > > >>
        > > >>
        > > >>
        > > >>     ===========================================
        > > >>
        > > >>     José Carlos Cordeiro
        > > >>
        > > >>     Diretoria Técnica - Laboratório Central
        > > >>
        > > >>     Centro Técnico - Curitiba
        > > >>
        > > >>     Rodovia PR-092, 1303, Abranches, 82130-570 Curitiba-PR
        > > >>
        > > >>     Votorantim Cimentos
        > > >>
        > > >>     [EMAIL PROTECTED]
        > > <mailto:[EMAIL PROTECTED]>
        > > >>
        > > >>     www.votorantimcimentos.com.br
        > > >>
        > > >>     Fone: + 55 041 3355-1380
        > > >>
        > > >>     Fax:   + 55 041 3355-1358
        > > >>
        > > >>     ===========================================
        > > >>
        > > >>
        > > >>
        > > >>
        > >
        > >
        >
        >
        >
        >
        >
        
        
        
        
        


Reply via email to