Dear Mikko,

Your XRD pattern is well approximated by an orthorhombic Pbcn structure with 
lattice parameters a=5.187,   b=5.607,   c=5.311, which may present a new 
anisotropically disported polymorph of cubic (Ce?,Sn?)O4.

Best regards,
Leonid
 

*******************************************************
Leonid A. Solovyov
Institute of Chemistry and Chemical Technology
660049, K. Marx 42, Krasnoyarsk, Russia
http://sites.google.com/site/solovyovleonid
*******************************************************



On , Leonid Solovyov <[email protected]> wrote:
 
Dear Mikko,

Your XRD pattern is well approximated by an orthorhombic Pbcn structure with 
lattice parameters a=5.187,   b=5.607,   c=5.311, which may present a new 
anisotropically disported polymorph of cubic (Ce?,Sn?)O4.

Best regards,
Leonid
 

*******************************************************
Leonid A. Solovyov
Institute of Chemistry and Chemical Technology
660049, K. Marx 42, Krasnoyarsk, Russia
http://sites.google.com/site/solovyovleonid
*******************************************************



On Friday, October 25, 2013 2:33 PM, Mikko Heikkilä 
<[email protected]> wrote:
 
Dear Rietvelders,
 
I decided to completely embarrass myself and ask you a simple phase 
identification question. I’ve had some trouble in trying to figure out what’s 
going on with one measurement done in our lab. The sample is a ~30nm film heat 
treated in air at 500C, composition is Ce:Sn in close to 1:1 ratio plus oxygen 
in addition to those. I can’t tell if there’s any very light elements as we 
only have EDX data at the moment, and the actual amount of O is still unclear 
due to 3-4nm of native SiO2 under the sample and I don’t have any XPS/RBS/SIMS 
profile data yet. I can’t find anything from our databases that would fit even 
remotely close to the measured data. (we have ages old PDF2 but I’ve imported 
every CeOx, SnOx and CexSnyOz structure I could find from latest ICSD). 
Indexing is a bit frustrating as well since I can’t be sure if it’s a single 
phase, and I don’t have too much experience with unknowns anyway. 
 
The measurement was done in grazing incidence mode with 1deg incident angle (it 
seems that there was some 0.014deg of 2theta shift back then).  I’ve done 
rocking curve measurements from the first six reflections, based on that it 
doesn’t seem to be textured so there shouldn’t be reflections missing due to 
that (particle statistics is obviously a different matter…). When measuring 
with different incident angles (from 0.25 to 3.75 2th) the diffractograms don’t 
seem to change, so there’s probably no separate layers but one homogeneous 
matter. The data is found here for those interesting in trying: 
http://www.helsinki.fi/~mwheikki/temp/  And before you ask, there’s no 
reflections below the one at 23.5 2th. And it’s a Cu tube.
 
I really appreciate any effort and time any of you might spend with the data. 
I’m currently trying to find something from the literature but no success so 
far. Hopefully you can make me feel stupid and find out the easy solution 
before I do J
 
Have a nice weekend!
 
BR,
Mikko
 
---
Mikko Heikkilä, M.Sc., Laboratory engineer
Laboratory of Inorganic Chemistry
Department of Chemistry
P.O. Box 55 (A.I. Virtasen aukio 1)
FI-00014 University of Helsinki
 
phone:   +358919150216
mobile:  +358504160572
email: [email protected]
 
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <[email protected]>
Send commands to <[email protected]> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++
Please do NOT attach files to the whole list <[email protected]>
Send commands to <[email protected]> eg: HELP as the subject with no body text
The Rietveld_L list archive is on http://www.mail-archive.com/[email protected]/
++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++++

Reply via email to