On Sun, Jul 03, 2016 at 12:33:04PM +0200, Andrea Baldoni wrote: > Hello. > I repeated the experiment with a better setup, I also added > some alloys that are already arrived. So far, a really "low" > EMF solder hasn't been identified.
> Measurements have been done between water ice point and boiling > point with Agilent 34401A. I don't expect the curves be linear, > but here it's assumed they are. > Copper - Sn96.5/Ag3/Cu0.5 -> 3.35uV/K > Copper - Sn95.5/Ag3.8/Cu0.7 -> 3.22uV/K > Copper - Sn60/Pb40 -> 3.34uV/K > Copper - Pb92.5/Sn5/Ag2.5 -> 3.02uV/K > Copper - Brass -> 3.30uV/K > I am waiting for Sn96/Ag4, Sn99/Cu1. Any plans on testing Sn42/Bi57.6/Ag0.4 ? Thanks, Herbert > Best regards, > Andrea Baldoni > _______________________________________________ > volt-nuts mailing list -- [email protected] > To unsubscribe, go to https://www.febo.com/cgi-bin/mailman/listinfo/volt-nuts > and follow the instructions there. _______________________________________________ volt-nuts mailing list -- [email protected] To unsubscribe, go to https://www.febo.com/cgi-bin/mailman/listinfo/volt-nuts and follow the instructions there.