Thanks Bob.  I think I understand how to do that. I will give it a try today.

-Darin

At 07:26 AM 8/10/2004, you wrote:
Dear Darin & others,
The trick here is to realize the effect of the different site multiplicities. Moreover, remember that the constraint applies to the shifts & not the values. So start the site fractions with the right stereochemistry - you can put all Co in one site & all Fe in the other with the duplicate sites set to zero FRAC. Then put in constraint that forces amount of Fe lost from A-site to appear in the B-site and vise versa for the Co; a single constraint with 4 terms should suffice. The constraint factors will be 1.0 or 0.5 to account for the site multiplicity changes. All this assumes no vacancies - you can't really determine that from a single experiment, too many variables & not enough information.
Bob Von Dreele


________________________________

From: Darin Hoffman [mailto:[EMAIL PROTECTED]
Sent: Mon 8/9/2004 5:23 PM
To: [EMAIL PROTECTED]



Hello all:

I am currently working on a rietveld refinement of CoFe2O4 using GSAS. The
structural model I am using is
Site A 1/8, 1/8, 1/8
Site B 1/2, 1/2, 1/2
Oxygen site 1/4+d,1/4+d,1/4+d

On site A and B both Iron and Cobalt are present.

I am trying to create a constraint that forces the ratio of the Co:Fe to be
1:2 as well as force the fractional occupancies of each site to inverse
each other .  In other words percent Iron goes up percent Cobalt goes
down.  This part I have been able to do quite easily.  I thought I was able
to set up the 1:2 ratio constraint correctly but I don't believe the answer
because I am getting the Cobalt on both sites to have a Fraction value of
~0.28 and the Iron fraction to = ~ 0.57.  I know that I may have vacancies
but I don't believe both site should be the same.

Can anyone please tell me how to set up a chemical ratio constraint either
going through the EXPGUI or DOS interface?

Sincerely,

Darin Hoffman


################################################# Darin Hoffman, TSPA Research Intern, NPDF Lujan Neutron Scattering Center Los Alamos National Laboratory e-mail: [EMAIL PROTECTED] PH: 505-667-8704 #####################################################

#################################################
Darin Hoffman, TSPA
Research Intern, NPDF
Lujan Neutron Scattering Center
Los Alamos National Laboratory
e-mail: [EMAIL PROTECTED]
PH: 505-667-8704
#####################################################




Reply via email to