Dear Gustavo,

the cell (space group Pna21) should be:

4.834 x 8.3096 x  8.9353

Structure:


 Al1    0.1778 0.8383 0.6466 
 Al2    0.330700 0.024500 0.3775 
 Al3    0.313800 0.350200 0.5713
 Al4    0.315600 0.657600 0.3734 
 O1    0.479600 0.852900 0.4977 
 O2    0.508500 0.508900 0.505 
 O3    0.162700 0.163200 0.2429 
 O4    0.154400 0.495300 0.2656 
 O5    -0.020200 0.323100 0.5166 
 O6    0.163800 0.841000 0.2708 


I hope this will help you,
good luck,