> Dear All,
> 
> I am trying to carry out Rietveld refinement on a sample that has 
> very obvious peak shape variation; probably due to subcell and 
> supercell peaks. I believe there is a way to deal with this in GSAS, 
> but I can't quite work out the best way.
> 
> I'd be grateful for any tips
> 
> Caroline
> 
> 
> Caroline Kirk

(Not sure if the following is consider hypocritical given I have
posted on a previous occasion questioning if spherical harmonics
for powder diffraction are a new form of evil)

This may not be helpful to your specified query but if you have a Bruker 
XRD with Topas Rietveld software - Topas has an option to apply spherical 
harmonics not only to Preferred orientation, but also anisotropic
peak broadening, peak displacements (e.g., due to stress/strain) and 
some other parameters as well.

       http://www.bruker-axs.com

-----

You apply the following style of Topas command to generate the 
spherical harmonics for peak anisotropy (this is on an older
beta-test version of the software):

prm p1 0.01311 min 0.0001 
   spherical_harmonics_hkl sh1
      sh_order 6 
      lor_fwhm = sh1 p1;

(run some refinement cycles and job done)

----------

This was tried with some very nasty and complex peak anisotropy
in a new Titanate shear structure (I.E. Grey, L.M.D. Cranswick, C. Li, 
T.J. White and L.A. Bursill, "New M3O5-Anatase Intergrowth Structures 
Formed during Low-Temperature Oxidation of Anosovite" Journal of solid 
State Chemistry, 150, 128-138 (2000).)

Results follow (refinement needed quite severe bond length restraints to
stop oxygens wandering around):

---

Harmonic Order Used     R_wp (%)         R_bragg (%)

No Spherical Harmonics  13.13              7.12
2nd order               9.38               3.43
4th order               9.63               3.60
6th order               8.76               3.19
8th order               7.89               2.11

----

Harmonic Order Used    B Titanium (1-6)    B Oxygen (1-11)

No Spherical Harmonics  -0.9258               3.5033
2nd order                0.2557               0.8148
4th order                0.3000               0.7615
6th order                0.3831               1.2392
8th order                0.2967               0.6551


-------

(I am not sure what other Rietveld programs allow this as well?)

Lachlan.

-- 
Lachlan M. D. Cranswick

Collaborative Computational Project No 14 (CCP14)
    for Single Crystal and Powder Diffraction
Daresbury Laboratory, Warrington, WA4 4AD U.K
Tel: +44-1925-603703  Fax: +44-1925-603124
E-mail: [EMAIL PROTECTED]  Ext: 3703  Room C14
                           http://www.ccp14.ac.uk

Reply via email to