>> Dear All,
>>
>> I am trying to carry out Rietveld refinement on a sample that has
>> very obvious peak shape variation; probably due to subcell and
>> supercell peaks. I believe there is a way to deal with this in GSAS,
>> but I can't quite work out the best way.
>>
>> I'd be grateful for any tips
>>
>> Caroline
>>
>>
>> Caroline Kirk
>
........
>This may not be helpful to your specified query but if you have a Bruker
>XRD with Topas Rietveld software - Topas has an option to apply spherical
>harmonics not only to Preferred orientation, but also anisotropic
>peak broadening, peak displacements (e.g., due to stress/strain) and
>some other parameters as well.
>
>       http://www.bruker-axs.com
>
...............
>
>(I am not sure what other Rietveld programs allow this as well?)
>Lachlan M. D. Cranswick


The program Maud (see my web pages) also models anisotropic peak broadening
using the Popa (see on J. Appl. Cryst. of 1998, May-June?) model. It's an
advanced harmonic expansion method were the Laue group of the phase imposes
some obvious constraints on the harmonics to respect symmetries.

There is another problem to know.  Is the observed strange peak shape
simply anisotropy or there are other effects, like superstructure peak
broadening, asymmetry and peak displacement by faulting etc.?
In that case you need some special treatments (a.k.a Warren theories for
twin, stacking faults and/or antiphase boundary). Maud can be used in this
case but the actual general model only works for bcc, fcc, hcp structures.
No general approach available up to now.

Probably you may give some more information about the material and what
kind of strange peak shape you are observing.

                Best regards,
                        Luca Lutterotti



-----------------------Luca Lutterotti----------------------------
 Dipartimento di Ingegneria dei Materiali, Universita' di Trento,
 via Mesiano 77, 38050 Trento, Italy

 e-mail address : [EMAIL PROTECTED]
 Home page : http://www.ing.unitn.it/~luttero
 Mirror: http://www.ccp14.ac.uk/ccp/web-mirrors/lutterotti/~luttero/

 Phone number :+39-0461-88-2414
-Fax : +39-0461-88-1977-----------------------------------------


Reply via email to